1、聚酯中添加季戌四醇前后生產對比報告一、說明2006年9月年保后,在聚酯生產中添加季戌四醇(AD21),旨在提升POY后加工染色性能。針對添加AD21前后紡絲生產工藝控制、產品品質指標、產量等級率及廢絲量等各項指標進行比較。二、聚酯生產比較(一)產量及熔體品質指標時段月份產量(T/D)IVCOOH(meq/kg)b值L值熔點()ASH%(%)DEG%(%)添加AD21前(1)0603431.8 0.6835 35.27 2.57 73.4 260.0 0.342 1.347 0604433.3 0.6834 34.45 2.50 73.3 260.0 0.341 1.341 0605432.9
2、0.6831 34.89 2.74 74.8 260.0 0.342 1.336 0606429.6 0.6832 35.73 2.83 74.7 260.0 0.339 1.332 0607428.0 0.6835 34.30 2.90 75.3 260.0 0.333 1.327 平均值431.1 0.6834 34.93 2.71 74.3 260.0 0.339 1.337 添加AD21后(2)0610422.0 0.6833 30.45 3.16 73.3 259.8 0.344 1.345 0611450.2 0.6827 32.14 3.34 73.9 260.0 0.339 1
3、.344 0612451.6 0.6832 32.74 3.14 73.0 260.0 0.335 1.347 0701444.6 0.6828 34.07 3.15 74.3 260.0 0.333 1.356 0702404.2 0.6839 32.67 3.05 74.7 260.0 0.338 1.357 平均值441.3 0.6831 31.77 3.21 73.4 259.9 0.339 1.345 差異(2-1)10.2 -0.0003 -3.15 0.51 -0.9 -0.1 0.000 0.008 備注:8月下旬至9月上旬年保檢修,故不取此2月份數(shù)據(jù);A、 從IV分析值看,添
4、加AD21前后,熔體IV控制值相當,無明顯差異;B、 添加AD21前(年保前),R-3100真空管道堵塞嚴重,真空效果差,制程必須控制酯化高酸價來滿足生產需求,故切片COOH值相應會比年保后略高;C、 切片B/L值變化主要受PTA品質影響較大;年保后切片改批,B值控制中心改變。D、 從分析平均值看,添加AD21后,切片熔點有微降,但不明顯;E、 切片ASH%值主要與外添加量有關;DEG%含量主要與反應自生產量與外添加量有關;(二)工藝參數(shù)與控制對比添加AD21前,為達到相同的熔體粘度,添加AD21后,縮聚段的真空負荷略有加大,其余工藝參數(shù)基本無明顯差異;(三)過濾器壓升及使用周期添加AD21后
5、:(1)酯化物過濾器F-2230使用情況無明顯差異;(2)熔體過濾器F-3340使用初壓上升、壓升變快,使用周期變短。以420T/D產能為例,使用初壓由37kg/cm2上升至40.5kg/cm2,增高約34kg/cm2;濾芯日壓差上升值增加約0.3kg/cm2(0.420.76);過濾器使用周期大大縮短。(四)產量等級率CP1月份聚酯月產量(噸)切片月產量(噸)A級(噸)B級(噸)C級(噸)A級率(%)降級原因添加AD21前(1)060313385.750 2847.2 2844.0 0.0 3.2 99.98%A-3300皮斷裂,更換。060412999.474 2858.4 2858.4
6、0.0 0.0 100.00%060513418.533 3066.4 3066.4 0.0 0.0 100.00%060612888.761 3007.2 2924.0 76.8 6.4 99.35%6/11 P-3400跳停;6/16電網波動P-33/34跳停。060713266.654 2992.0 2992.0 0.0 0.0 100.00%平均值13191.834 2954.2 2937.0 15.4 1.9 99.87%添加AD21后(2)061013083.041 2040.8 2040.8 0.0 0.0 100.00%061113505.029 3323.2 3323.2 0
7、.0 0.0 100.00%061213999.245 3957.3 3957.3 0.0 0.0 100.00%070113782.013 4301.6 4301.6 0.0 0.0 100.00%070211319.348 2100.0 2100.0 0.0 0.0 100.00%平均值13137.735 3144.5843144.6 0.0 0.0 100.00%差異(2-1)-54.099 190.3 207.6 -15.4 -1.9 0.0013若扣除外部原因引起的降級,添加AD21前后聚酯生產A級率相當。三、紡絲生產比較(一)紡絲工藝、物性、斷紗、異常紗、CPF或組件壓升周期,以及
8、廢絲量等比較1、直紡線比較:以SP1之300D/72F、75D/36F、150D/96F及SP2之150D/144F年保前后同線同規(guī)格生產工藝與物性進行比較。項目單位添加AD21前添加AD21后添加AD21前添加AD21后添加AD21前添加AD21后添加AD21前添加AD21后線別L2L7L10L21批號13620130020301803000103184031004051340510030規(guī)格dtex/f528/72128/36262/96262/144噴絲板*L0.28*0.600.21*0.600.22*0.500.21*0.60組態(tài)8F400目+海砂10目170g+5F600目3F40
9、0目+(金屬砂20目220g)+5F1200目3F400目+(金屬砂30目140g+80目60g)+5F800目金屬砂60目20g+30目160g金屬砂30目140g紡絲溫度281284291292287287291.5289.5熔體溫度294293293.9294.7291291.1292289紡速m/min32503250318032003270328531253175GR1m/min32703270321832203300331531583208GR2m/min32763276322632283313333031633213油劑型號TT-2707L-113TT-2707TT-2597纖度
10、dtex533.6538.4140.8143.5280.6280.6266.6268.0強度%2.292.242.562.462.572.522.452.38伸長%138.4144.9139.9144.3134.7142.7134.4140.4U值%0.940.890.880.871.061.121.251.24OPU%0.340.330.330.340.370.370.410.42斷紗次/天2.02.54.74.16.47.56.08.1異常紗錠/天6.08.03.92.45.74.71.42.7組件壓升kg/天0.300.750.330.881.001.391.01.4DTY后加工簡要說明
11、斷紗1.9條,M率98.5%,外觀略有毛絲斷紗2.2條,M率98.6%,外觀毛絲有改善斷紗2.6條,M率98.7%斷紗3.2條,M率98.8%斷紗1.5條,M率98.6%,外觀有短毛絲斷紗1.9條,M率98.7%,外觀短毛絲有改善斷紗1.3條,M率99.1%斷紗1.7條,M率99.1%(二)產量等級率及廢絲率比較1、直紡線產量等級率比較(6月份SP1/2兩次外部原因全線跳車降級多,改取4月份數(shù)據(jù))(1)產量等級率比較表SP1直紡月份月產量(噸) AA級(噸) AT級(噸)A1級(噸) B級(噸) C級(噸)AA率添加AD21前(1)2006046,553.966,310.01128.5050.
12、3546.0219.0896.282006056,559.726,364.58105.7830.2640.3418.7697.032006076,387.776,147.83131.6348.1342.2817.9196.24小計19,501.4518,822.42365.91128.74128.6355.7596.52添加AD21后(2)2006106,718.596,455.81138.6844.3349.2330.5496.092006116,248.005,985.01142.6440.5743.2536.5495.792006126,258.126,018.59126.3051.15
13、32.3129.7896.17小計19,224.7118,459.41407.61136.05124.7996.8596.02差異(2-1)-276.74-363.0141.707.31-3.8441.10-0.50 廢絲率比較(取年保前后各3個月數(shù)據(jù),6月價直紡跳車兩次改取4月數(shù)據(jù))課別SP1SP2項目月份產量(噸)廢絲量(噸)廢絲率(%)產量(噸)廢絲量(噸)廢絲率(%)添加AD21前(1)2006047,789.862 127.361.63%2404.1445.841.91%2006057,870.247 116.851.48%2346.8346.181.97%2006077,773.5
14、91 120.051.54%2341.4044.481.90%月平均7,811.233 121.421.55%2,364.119 45.501.92%添加AD21后(2)2006108,141.892 147.841.82%2480.0850.472.04%2006117,629.598 128.551.68%2520.5752.922.10%2006127,506.915 125.601.67%2457.7350.312.05%月平均7,759.468 134.001.73%2,486.126 51.232.06%差異=(2)-(1)-51.7712.580.17%122.015.730.14%從上述年保添加AD21前后生產各項數(shù)據(jù)比較來看,相同規(guī)格直紡在生產工藝條件控制基
溫馨提示
- 1. 本站所有資源如無特殊說明,都需要本地電腦安裝OFFICE2007和PDF閱讀器。圖紙軟件為CAD,CAXA,PROE,UG,SolidWorks等.壓縮文件請下載最新的WinRAR軟件解壓。
- 2. 本站的文檔不包含任何第三方提供的附件圖紙等,如果需要附件,請聯(lián)系上傳者。文件的所有權益歸上傳用戶所有。
- 3. 本站RAR壓縮包中若帶圖紙,網頁內容里面會有圖紙預覽,若沒有圖紙預覽就沒有圖紙。
- 4. 未經權益所有人同意不得將文件中的內容挪作商業(yè)或盈利用途。
- 5. 人人文庫網僅提供信息存儲空間,僅對用戶上傳內容的表現(xiàn)方式做保護處理,對用戶上傳分享的文檔內容本身不做任何修改或編輯,并不能對任何下載內容負責。
- 6. 下載文件中如有侵權或不適當內容,請與我們聯(lián)系,我們立即糾正。
- 7. 本站不保證下載資源的準確性、安全性和完整性, 同時也不承擔用戶因使用這些下載資源對自己和他人造成任何形式的傷害或損失。
最新文檔
- 現(xiàn)代醫(yī)學與中醫(yī)結合的三叉神經痛方案
- 吉林大學《水力學》2021-2022學年第一學期期末試卷
- 公路維修施工材料選擇方案
- 吉林大學《素描人體》2021-2022學年第一學期期末試卷
- 預拌混凝土驗收及賠償協(xié)議
- 鋼鐵生產工藝優(yōu)化施工方案
- 農民合作社發(fā)展實施方案
- 同步測控優(yōu)化設計2024年七年級數(shù)學上冊第一章有理數(shù)1.4有理數(shù)的乘除法1.4.1第1課時有理數(shù)的乘法知能演練提升新版新人教版
- 2024高考物理一輪復習課時作業(yè)四十二光的波動性電磁波相對論含解析新人教版
- 2024-2025學年新教材高中化學第八章化學與可持續(xù)發(fā)展第1節(jié)第2課時煤石油和天然氣的綜合利用學案新人教版必修2
- 蒸汽鍋爐可行性方案
- 煤焦酚-安全技術說明書MSDS
- 【課件】第二課時光合作用的原理和應用課件-2023-2024學年高一上學期生物人教版(2019)必修1
- 焚燒爐RTO操作規(guī)程
- 數(shù)據(jù)庫安全事件響應機制
- 涉僑法律知識講座
- 少先隊輔導員筆試題
- NCCN成人癌痛指南
- 地面沉降干涉雷達監(jiān)測規(guī)范
- (許濟洛平)洛陽市2023-2024學年高三第二次質量檢測 英語試卷(含答案)
- 醫(yī)院培訓課件:《重癥患者安全轉運》
評論
0/150
提交評論